TEMA Tubesheet Design & Tube-to-Tubesheet Joint Integrity (Welded vs Expanded)
TEMA and ASME Section VIII tubesheet mechanical thickness design, roller expanded vs seal-welded vs full-strength welded tube joints.
1. Theoretical Foundations & Engineering Mechanics
Tubesheet Thickness & Tube-to-Tubesheet Joints
The tubesheet acts as the structural barrier separating shellside and tubeside fluids. It must withstand high differential pressures, thermal expansion loads, and bolt moments without excessive deflection that could cause gasket blowout or tube joint leakage.
1. Mechanical Sizing Codes:
- TEMA Standards (Section 5): Provides empirical thickness formulas based on maximum bending stress and shear stress across the drilled ligament.
- ASME Section VIII Div 1 (Part UHX): Modern analytical approach treating the tubesheet as a circular plate elastically supported by the shell, channel, and elastic foundation of the tube bundle.
2. Tube-to-Tubesheet Joint Methods:
- Roller Expanded: Tubes mechanically expanded into tubesheet holes. Serrated annular grooves (two grooves, each $3.2\text{ mm}$ wide $\times 0.4\text{ mm}$ deep) provide mechanical anchoring and pull-out resistance ($f_r$). Suitable for moderate pressures and non-toxic services.
- Seal Welded: Tubes expanded, followed by a light autogenous or single-pass fillet weld. Prevents micro-leakage in hydrogen or volatile hydrocarbon service.
- Full Strength Welded: Two-pass or multi-pass fillet/groove weld designed to carry the full axial tube load without relying on mechanical expansion. Mandatory for high-pressure exchangers ($P > 70\text{ bar}$), severe cyclic thermal duties, and lethal/toxic fluids (hydrogen sulfide, phosgene).
2. Governing Equations & Mathematical Formulation
$$\text{TEMA Bending Thickness: } T_b = \frac{F G}{2} \sqrt{\frac{P}{\eta S}}$$
$$\text{TEMA Shear Thickness: } T_s = \frac{0.31 D_L}{\left(1 - \frac{d_o}{P_t}\right)} \left( \frac{P}{S} \right)$$
$$\text{Governing Tubesheet Thickness: } T_{ts} = \max(T_b, T_s) + C_A$$
$$\text{Ligament Efficiency: } \eta = \frac{P_t - d_h}{P_t}$$
• Allowable stress $S$ is evaluated at design metal temperature from ASME Section II Part D.
• Ligament efficiency $\eta$ accounts for metal removed by drilling tube holes.
• Corrosion allowance ($C_A$) is added only to the process-wetted side(s).
• Relying solely on roller expansion for hydrogen or cyclic thermal service, resulting in premature tube joint leaks.
• Over-expanding tubes during roller rolling ($> 8\%$ wall reduction), which work-hardens the tube, induces stress corrosion cracking (SCC), and distorts adjacent tubesheet holes.
• Overlooking differential thermal expansion in fixed tubesheet exchangers, which can shear the tube-to-tubesheet weld.
3. Applied Engineering Worked Example
Design Pressure: $P = 4.0\text{ MPa}$ ($40\text{ bar}$), Shell Gasket Diameter $G = 700\text{ mm}$
Material: SA-516 Gr 70 Carbon Steel, Allowable Stress $S = 138\text{ MPa}$, TEMA factor $F = 1.0$
Tubes: $P_t = 31.75\text{ mm}$, hole diameter $d_h = 25.65\text{ mm}$, Corrosion Allowance $C_A = 3.0\text{ mm}$
-
Calculate Ligament Efficiency ($\eta$):
$$\eta = \frac{P_t - d_h}{P_t} = \frac{31.75 - 25.65}{31.75} = \frac{6.10}{31.75} = 0.1921$$ -
Calculate TEMA Bending Thickness ($T_b$):
$$T_b = \frac{1.0 \times 700}{2} \sqrt{\frac{4.0}{0.1921 \times 138}} = 350 \times \sqrt{\frac{4.0}{26.51}} = 350 \times \sqrt{0.1509} = 350 \times 0.3884 = 135.9\text{ mm}$$ -
Add Corrosion Allowance:
$$T_{final} = T_b + C_A = 135.9 + 3.0 = 138.9\text{ mm}$$ -
Engineering Specification:
Specify standard plate stock thickness of $140\text{ mm}$ (5.5 inches). Because $T > 100\text{ mm}$, ultrasonic testing (UT) per ASME SA-578 is required to detect laminations before drilling.
Interactive Practice Drill: TEMA Tubesheet Design & Tube-to-Tubesheet Joint Integrity (Welded vs Expanded)
Completed this lesson?
Record your study progress, build your daily streak, and unlock +25 XP toward your next engineering tier.
Connected ChemProCal Tool